Conductivity of Aerospace Aluminum

Eddy current inspection to verify heat treatment, confirm the temper and master the six factors that alter every reading — within the framework of AMS2658D.

METHOD Eddy current (ET) INSTRUMENT FOERSTER SIGMATEST 2.070 STANDARDS ASTM E1004 · AMS2658D
Portrait of Inspector Pepe Grietas, LLOG's non-destructive testing assistant
Ask Inspector Pepe Grietas This conductivity lesson is part of his knowledge base. Ask him to explain a section, redo the calculations with your inspection data, or help you interpret a reading.
Ask Pepe
01 · The concept

What is conductivity and why does aerospace measure it?

Electrical conductivity is the ease with which electrons move through a material. The more freely they flow, the higher its conductivity.

In the aerospace industry this measurement is a safety tool: it lets you verify the heat treatment of aluminum structures, confirm the corrosion-resistant temper in 7xxx alloys and detect heat damage — all non-destructively, without compromising the part. It is the basis of specifications such as AMS2658D.

All matter is made of atoms with a nucleus of protons and neutrons surrounded by orbiting electrons. The flow of those electrons through the material is an electric current. The relative ability of a metal's atoms to allow that flow is precisely its conductivity: a physical property that depends on the composition, the crystal structure and the treatment condition of the material.

Think of it this way

Conductivity is a highway for electrons. In a pure metal the highway is clear and current flows fast (high conductivity). Each alloying atom is like a car parked in a lane: it gets in the way. That is why a little alloying element slows traffic a lot — and why conductivity gives away the composition and condition of the material.

In non-destructive testing, a coil excited with alternating current induces eddy currents in the part. The material's conductivity changes the complex impedance of the coil; the instrument converts that impedance change into a conductivity value. That is why it is an indirect measurement, sensitive to anything that alters the path of the induced currents.

02 · Units and standards

The copper scale: % IACS

Every metal is assigned a conductivity value on a scale relative to pure annealed copper: the International Annealed Copper Standard.

100 %IACS
Pure annealed copper (reference)
58 MS/m
SI equivalent of 100 %IACS
1–112 %IACS
Typical range of common metals

The IACS standard defines a copper bar 1 meter long with a 1 mm² cross-section, held at 20 °C, with a resistance of 0.017241 Ω, which equals 100 %IACS. The SI unit is the siemens per meter (S/m); by convention, 100 %IACS = 58 MS/m.

The international primary standards are kept at NIST (USA) and NPL (UK), with an accuracy close to 0.2 %IACS, and are cross-calibrated against each other to maintain traceability. Secondary standards — the ones that normally come with a field instrument such as the SIGMATEST — reach a typical accuracy of 0.35 %IACS.

Quick conversion: %IACS = (σ in MS/m ÷ 58) × 100. The full %IACS ↔ MS/m converter with temperature normalization is in Module 01.
03 · What alters the reading

Six factors that affect the measurement

Measured conductivity does not depend on the material alone: geometry, temperature and test frequency change the result. Knowing them is the difference between a valid reading and an unjustified rejection.

A

Chemical composition

Small amounts of alloying elements reduce conductivity drastically.

B

Heat treatment

Temper and cold work change the structure — and conductivity with it.

C

Temperature

The higher the temperature, the more the atoms vibrate and the lower the conductivity.

D

Thickness

Below 3× the standard depth of penetration the reading is no longer reliable.

E

Cladding

The cladding layer (Alclad) shifts the reading depending on the frequency used.

F

Curvature

Convex and concave surfaces require correction factors.

Factor A · Chemical composition

The alloying element rules

Conductivity usually drops dramatically with very small amounts of an alloying element. The purity of the base metal matters less than what is added to it.

Pure copper conducts at 100 %IACS, but a 90-10 copper-nickel drops to ~9.7 %. Commercially pure titanium is close to 3 %IACS; alloyed as Ti-6Al-4V it drops to ~1 %. This sensitivity is what makes conductivity useful for sorting and verifying materials.
Factor B · Heat treatment

Why hardness and conductivity go together

The correlation between hardness and conductivity is the basis of heat-treatment verification by eddy current. But neither one is enough on its own.

Heat treatment and cold work rearrange the crystal structure of the alloy. The annealed (O) form of any alloy has the most regular structure — and therefore the highest conductivity. When the alloy is aged or hardened, conductivity changes measurably: an annealed 2014 is around 50 %IACS, while in the 2014-T4 condition it drops to ~30 %IACS.

Key rule: a given conductivity value does not imply a single hardness value. Both measurements are needed to establish the true condition of the material. That is why AMS2658D requires hardness and conductivity — the SIGMATEST 2.070 covers conductivity; the SONODUR 3 (UCI method) provides the Vickers hardness that completes the assessment.

In aerospace aluminum alloys, this correlation is the practical tool for confirming that a part received the correct heat treatment without destroying it: measure conductivity in the field, compare it against the specification's acceptance bands, and confirm with hardness where needed.

Factor C · Temperature

Every degree counts

As temperature rises, atoms vibrate with greater amplitude and interfere with the movement of electrons. The result: conductivity decreases.

69 %IACS
CP aluminum at −10 °C
62 %IACS
Same aluminum at 20 °C
↓ as T rises
Higher temperature, lower conductivity

The relationship is inverse and far from negligible: the same commercially pure aluminum goes from 69 %IACS at −10 °C to 62 %IACS at 20 °C. The acceptance bands in the standards are referenced to 20 °C, so every reading must be normalized to that temperature before comparing it.

On the SIGMATEST 2.070 temperature compensation is automatic: each instrument comes with a default coefficient and the user can define a specific one for their application. The reading is standardized to 20 °C internally — but the inspector must remember to verify calibration when the ambient temperature changes significantly during the shift.
Factor D · Thickness and penetration

Standard depth of penetration calculator

Eddy currents attenuate exponentially with depth. For a valid reading, the material must be at least three times the standard depth of penetration (δ).

Think of it this way

Eddy currents are like the echo of your voice in a cave: strong at the surface and weaker and weaker toward the bottom. The depth of penetration (δ) marks where they almost fade out. If the part is thinner than 3δ, the “echo” bounces off the far side and contaminates the reading — like trying to measure the depth of a pool that is really a puddle.

35.0%
mm
Standard depth δ
0.46 mm
Minimum thickness (3δ)
1.37 mm
Is your part thicker than the depth the currents reach?
Current penetration (3δ)0 mm
The copper bar fades toward its tip: that is how the currents fade with depth. If your part is longer than that bar, the far side does not interfere.
Enter a thickness to evaluate whether the measurement is valid.
Formula: δ = 1 / √(π · f · μ · σ)  — where f is the frequency (Hz), μ the magnetic permeability (μ₀ for non-ferromagnetic metals) and σ the conductivity (S/m). In the field the equivalent form δ = 660 / √(σ · μr · f) mm is often used, with σ in %IACS and f in Hz (IAEA TCS-48): at 60 kHz and 35 %IACS it gives 0.46 mm, the same as here.

The thickness ≥ 3δ rule is conservative: it holds for thick parts with large probes (plane-wave field); with real probes the currents attenuate somewhat faster, so 3δ is a safe minimum (at 3δ the current density is ≈5 % of the surface value). Below ~½ of the minimum thickness, consistent results are no longer possible even with correction factors.
Materialδ @ 60 kHzMin. (3δ)δ @ 500 kHzMin. (3δ)
Al alloys (35 %IACS)0.46 mm1.4 mm0.16 mm0.47 mm
304 stainless steel (2.5 %IACS)1.71 mm5.1 mm0.59 mm1.8 mm
Ti-6Al-4V (1 %IACS)2.70 mm8.1 mm0.94 mm2.8 mm
Factor E · Cladding

Why procedures are written at 60 kHz

Aluminum alloys are often produced in Alclad form: an alloy sheet (e.g. 2014) with a thin cladding of pure aluminum — typically up to 0.005″ — to resist corrosion.

That cladding conducts differently from the base metal, so the reading is split between the two according to how much of the eddy current energy is dissipated in the cladding — and that depends on frequency:

Think of it this way

Measuring conductivity on clad material is like taking someone's temperature through a coat: at low frequency you mostly “feel” the body (the base metal, which is what you care about); at high frequency you only feel the coat (the cladding). That is why procedures are written at 60 kHz.

At 60 kHz recommended

  • Depth of penetration in pure aluminum ≈ 0.014″.
  • ~25 % of the energy is dissipated in the cladding.
  • The reading is weighted toward the base metal — which is normally what matters.

At 500 kHz caution

  • Depth of penetration ≈ 0.005″.
  • ~70 % of the energy is dissipated in the cladding.
  • The reading is weighted toward the cladding, not toward the material you want to evaluate.
Standards implication: the higher the frequency, the greater the effect of variations in cladding thickness. Results on clad material vary drastically with frequency, and most procedures were developed at 60 kHz. This explains Note 8.5 of AMS2658D: conductivity limits were removed from Table 2 because they were based only on a 60 kHz meter — for other frequencies the manufacturer's correction tables must be used.
Factor F · Curvature

Calibrated for flat surfaces

Eddy current conductivity meters are calibrated for use on flat surfaces. Measuring on curved surfaces requires care to maintain accuracy.

SituationMain effectMitigation
Concave surfaceProbe lift-offThe instrument compensates up to a limit; watch the lift-off at the center of the probe
Convex surfaceIndicated conductivity drops as the radius falls below ~3″Apply curvature correction tables
General rule—Lower frequencies give better results (except on thin-wall tubing)
On the SIGMATEST 2.070: if the conductivity of the reference piece is known, the curvature error is corrected by multiplying the reading by a correction factor, and the corrected value is shown on the display. Shielded probes also reduce edge effects.
Summary · Frequency decision

How to choose the test frequency

Three factors — thickness, conductivity and cladding — come together in a single practical decision: which frequency to use.

Low frequency e.g. 60 kHz

  • General inspection of high-conductivity materials.
  • Clad aluminum (Alclad) and similar materials.
  • When existing specifications based on 60 kHz govern curved, thin or clad material.
  • When the surface is rough, corroded or oxidized and does not represent the base material.

High frequency up to 960 kHz

  • Thin materials — thickness less than 3× the standard depth of penetration.
  • Low-conductivity materials (Ti alloys, high-alloy steels).
  • To separate low-conductivity materials from each other.
To separate low-conductivity materials, raise the frequency. To separate high-conductivity materials, lower it. The SIGMATEST 2.070 offers five frequencies — 60 / 120 / 240 / 480 / 960 kHz — maintaining accuracy even at 960 kHz for very thin parts.
Applied · Aluminum families

The aluminum families and how to inspect them

Aluminum is grouped into series according to its main alloying element. The key distinction for the inspector is whether the alloy is heat-treatable: that decides what conductivity can verify.

Inspection rule: in heat-treatable alloys (2xxx, 6xxx, 7xxx) conductivity verifies the temper condition against the AMS2658D bands. In non-heat-treatable alloys (1xxx, 3xxx, 5xxx) conductivity confirms the identity of the material and detects mix-ups, but strain hardening (H tempers) is confirmed with hardness, not conductivity.

The 7xxx case: conductivity rises with overaging

This is the flagship application. High-strength 7xxx alloys are tempered to peak hardness (T6), but that condition is susceptible to stress corrosion cracking (SCC). Overaging the part to T73 or T76 gains SCC resistance at the cost of some mechanical strength — and conductivity increases measurably. That is why conductivity is the non-destructive method for confirming that a part received the corrosion-resistant temper.

The mental trap

Back to the highway: in the T6 temper the obstacles (fine precipitates) are spread across every lane — they slow the current (low conductivity) but anchor the structure (high strength). With overaging, those obstacles gather into a few large clumps: they leave lanes clear (conductivity rises) but hold less (strength drops). That is why, in a 7xxx, more conductivity = more overaged = more corrosion resistance.

7075-T630.5–36 %
7075-T7338–43 %
7075-T7638–42 %
Scale 25–45 %IACS. Going from T6 (peak-aged) to T73/T76 (overaged), conductivity rises and SCC resistance increases; mechanical strength drops.
TemperConductivityBrinell min.Condition and use
T630.5–36.0 %135Peak-aged · maximum strength · susceptible to SCC
T7338.0–43.0 %125Overaged · resistant to stress corrosion cracking
T7638.0–42.0 %130Overaged · resistant to exfoliation

Conductivity bands and minimum Brinell hardness per AMS2658D, Table 1 (bare alloys). Conductivity measurement per ASTM E1004. Table 2 governs clad material.

Bare vs. clad, and the 6xxx case

Two warnings straight from AMS2658D that change how you inspect:

Clad material

  • Table 2 of AMS2658D has no conductivity band — only hardness. The pure aluminum cladding shifts the reading.
  • If you need a valid conductivity reading, measure at 60 kHz; on clad > 0.091″ the cladding may need to be removed locally.

6xxx series

  • AMS2658D gives the 6xxx conductivity values as reference only (Note 5).
  • To accept/reject 6xxx, use hardness as the primary criterion and conductivity as support.

Variations you will run into

Two readings on nominally identical material can differ. Before making a call, rule out these causes:

VariationWhy it happens
Same metal, different temper2024-O gives 46–51 % but 2024-T3 drops to 27.5–32.5 %. The temper rules.
Overlapping bandsNeighboring tempers share a range — which is why hardness is also needed to tell them apart.
CladdingReading weighted toward the cladding; no acceptance band for clad material.
Temperature not normalizedShifts the reading; normalize to 20 °C.
Thickness < 3δBelow the minimum the reading is no longer reliable.
Curved, rough or corroded surfaceDoes not represent the base material; apply a correction factor or recondition the surface.
Hardness + conductivity, always: a conductivity value does not pin down a single temper. The explicit example is 7050-T74 — AMS2658D accepts lower conductivities (38.0–39.9 %) only if the hardness does not exceed the maximum in its Table 3. The full catalog of 20 alloys / 69 tempers with their bands is in Module 02 (AMS2658D lookup).

The four most common in aerospace

Quick field reference. Each one teaches a different inspection lesson — acceptance values per AMS2658D (bare material, 60 kHz, normalized to 20 °C).

7075-T67xxx series · heat-treatable
Conductivity30.5–36.0 %
HardnessBrinell 135 · HRB 84
FormBare and clad
Use: highly loaded primary structure — wing skins, fuselage frames, fittings.
Caution: maximum strength but susceptible to SCC and exfoliation. Low conductivity confirms the T6; there is no conductivity band for clad material.
2024-T32xxx series · heat-treatable
Conductivity27.5–32.5 %
HardnessBrinell 100 · HRB 63
FormTypically Alclad
Use: fuselage skin. Excellent damage tolerance and fatigue resistance.
Caution: the lowest conductivity of the four. Almost always clad → measure at 60 kHz; Table 2 (clad) gives hardness only, with no conductivity band.
6061-T66xxx series · heat-treatable
Conductivity40.0–50.0 %*
HardnessBrinell 80 · HRB 47
FormBare and clad
Use: secondary structure, fittings, ducting. Good weldability and corrosion resistance.
Caution: *conductivity is reference only in AMS2658D (Note 5) → use hardness as the primary acceptance criterion.
7050-T747xxx series · heat-treatable
Conductivity40.0–44.0 %
HardnessBrinell 135 · HRB 82
FormThick plate and forgings
Use: thick sections — bulkheads, spars, landing gear components (AMS4050/4107/4108).
Caution: the Table 3 case — conductivities of 38.0–39.9 % are acceptable only if hardness ≤ 88/86/84 HRB depending on thickness. T74 = overaged to resist SCC in thick sections.
Let's put it into practice

Case study: accept or reject?

This is how the pieces come together. A conductivity reading without hardness — and without knowing the temper's band — can be misleading. Follow the reasoning.

Scenario: a 7075 part must be delivered in the T73 temper (resistant to stress corrosion cracking).
1
Look up the band. AMS2658D for 7075-T73: conductivity 38.0–43.0 % IACS, minimum Brinell hardness 125.
2
Prepare the measurement: normalize to 20 °C, use 60 kHz, confirm that thickness ≥ 3δ and that the surface is flat and representative.
3
You read conductivity = 34 % IACS. ⚠ It is outside 38–43 — and falls right in the T6 band (30.5–36 %).
4
You measure hardness with the SONODUR 3 = 138 Brinell. That is high, typical of T6, not T73.
Verdict: REJECT and refer to quality. The part is in the T6 condition, not T73: it has the strength of T6 but not the stress corrosion resistance the drawing requires — it received the wrong heat treatment. Note the lesson: with hardness alone, that 138 Brinell could have passed as a “good part”. It was conductivity that exposed the wrong temper.

Check your understanding

Test what you have learned: 5 random questions from a question bank. You will get an explanation for each one and, at the end, your score — with the option to try again with different questions.

Instrumentation

FOERSTER SIGMATEST 2.070

A portable eddy current instrument that measures the electrical conductivity of non-ferromagnetic metals from the complex impedance of the probe. The measuring range is set by calibration; on an unknown part, the instrument converts the impedance into a conductivity value shown on the display.

Its measurement quality meets Boeing (BAC 5651) and Airbus standards, as well as DIN 50994, ASTM E1004 and DIN EN 2004-1 — the same standards AMS2658D invokes for conductivity measurement.

Measuring range0.5–65 MS/m · 1–112 %IACS
Absolute accuracy±0.7 % @ 60 kHz, 14 mm probe
Resolution±0.1 % of measured value
Frequencies60 / 120 / 240 / 480 / 960 kHz
Lift-off compensationup to 750 µm
Temperature compensationautomatic to 20 °C
Applications

Where it is used in practice

Heat-treatment verification

Confirm that an aluminum alloy received the correct temper by comparing its conductivity against the AMS2658D bands.

Metal sorting

Separate and sort alloys, identify mixed materials and control purity through their conductivity signature.

Heat damage

Detect heat damage in wheels, engine components and lightning-strike areas, where heat alters the local conductivity.

Inspector's checklist

Before accepting a reading

✓Normalize the temperature to 20 °C (or confirm automatic compensation).
✓Verify calibration every hour of continuous operation.
✓Confirm that thickness ≥ 3× the standard depth of penetration.
✓Choose the frequency based on thickness, conductivity and cladding.
✓Apply a correction factor on curved surfaces.
✓Use a shielded probe to avoid edge effects.
✓Remember: conductivity and hardness together define the true condition.